Processing Procedure for Veromor Purge

  1. Mix 20% VeromorŪ Purge with medium flow HDPE, polypropylene or polymer you plan to process next. (This avoids polymer contamination).
    Virgin or regrind can be used.

  2. Starve screw & barrel.

  3. Temperature: Purge between 200-300 Celsius. Lower temperatures can be used. Ensure carrying polymer will flow through equipment at the lower temperatures.

  4. Polymer will be stiffer when mixed with VeromorŪ Purge

  5. RPM: You do not need to adjust the RPM in most cases prior to purging.
    It is recommended that the amp meter be observed to ensure purge is flowing satisfactorily through the barrel.


  6. Add VeromorŪ Purge polymer/purge mix to hopper & process through equipment

For Injection Moulding

For  Injection moulding. Add 1 – 2 kg (2.2-4.4 lb) of VeromorŪ Purge -XT polymer/purge mix for every 25 mm (1 inch) barrel diameter. If openings are smaller than 1.5mm use VeromorŪ Purge -XS.

For Hot Runner Systems

Add 1 – 2 kg (2.2-4.4 lb) of VeromorŪ Purge -XR polymer/purge mix for every 25mm (1 inch) barrel diameter.

For Extrusion Systems

Remove screen packs. Add 2 - 4 kg (2.2-4.4 lb) of VeromorŪ Purge -XS polymer/purge mix for every 25 mm (1 inch) barrel diameter.

Flush out VeromorŪ Purge  with polymer you plan to process next

Note:

If the screw & barrel have very bad carbonization, increase amount of VeromorŪ Purge processed through the barrel.VeromorŪ Purge can be used at higher addition level but must not exceed 35%

VeromorŪ Purge -XT and VeromorŪ Purge -XS are not suitable for hot runner systems.

 

 
  © 2006. All material within this web site is strictly copyright of PlastxWorld (Europe) Ltd. PlastxWorld USA, Inc. and PlastxWorld Inc. Any copying or reproduction of this information is strictly prohibited unless prior permission has been granted by PlastxWorld (Europe) Ltd. or PlastxWorld USA Inc or PlastxWorld Inc.